plate denitration catalyst |
The process that dry powder mixing method prepares tungsten trioxide plate denitration catalyst is as follows:
1. Put the titanium dioxide powder, stearate acid, AK sugars, methyl cellulose into the kneader, stir for about 10 minutes;
2. Add pulp slurry and stir for about 10 minutes;
3. Add silica sol solution and continually stir for 10 minutes;
4. Add the lactic acid, ammonia, ammonium metavanadate and suitable amount of deionized water into the mixed solution prepared above, then stir for about 1 hour for sufficiently reacting;
5. Add glass fiber and tungsten compound containing with tungsten trioxide (ammonium paratungstate, ammonium metatungstate ect.), stirring for about 30 minutes to prepare a catalyst mud;
6. Forming to generate the wet catalyst;
7. Dry the catalyst at 100 °C to remove excess free water;
8. Roasting, the purpose of it is: at the same time titanium dioxide crystal transition does not occurred, decompose the organic matter and active ingredient precursors; studies have shown that the active ingredient precursors and organic substances are decomposed completely at 400°C, the polymerization of vanadium pentoxide has been improved as the temperature increasing, but the titanium dioxide crystalline transition may occur, thus will cause the properties of catalyst reduced; therefore, calcination at the proper temperature, we can finally get the best active tungsten trioxide plate denitration catalyst.